高跟肉丝少妇A片在线-青青青国产在线观看免费-亚洲欧美另类在线图片区-欧美又粗又大xxxxbbbb疯狂-亚洲熟女少妇一区二区

Evolution of Die Wear and Sheared Edge Parameters in Trimming of DP980 Steel

2018-10-25 13:30:00
LUQIMENG
Original
2730

? Research Team at Oakland University
Saeid Nasheralahkami
Weitian Zhou
Scott Dawson
Daniel Kowalsky
Elizabeth Lekarczyk
Nan Wang
Sergey Golovashchenko


? Research  Team at  Ford

Lloyd Mason
Constantin Chiriac
Darryl Young
Raj Sohmshetty


? Research Team at US Steel

Brandon Hance
Ming Shi


? Research Team at AK Steel

Matt Folkner
Kavesary Raghavan
Yu-Wei Wang


? Research Team at PNNL

Guang Cheng
Kyoo Sil Choi
Xiaohua Hu
Xin Sun


? Sponsors: Ford, DOE VTO, FCA, NSF


? Introduction
? Traditional Trends in Trimming and Punching
? Mechanism of Fracture in Trimming of DP980
? Sheared Edge Stretchability for DP980 vs. DP600
? Die Wear Trend for Trimming of DP980
? Effect of Die Wear on Sheared Edge Stretchability
? Conclusions

Effect of Cutting Clearance on DP500 Edge


Mechanism of Fracture in Trimming

Equipment Utilized During Experimentation

Mechanism of Fracture in Shearing of DP980

Evolution of Burrs on Trimmed Edge - DP980

? The die wear test was conducted with 10% clearance
? After 35,000 cuts, the tool had some “wear”
? Experiments with various clearances were performed on new tool and 35k/10% tool


Typically, more wear is observed from the upper cutting tool due to excessive abrasion on the sheared edge of the blank during shearing and return motions.


Multiple publications on punch wear for punching round holes.


Excellent correlation of local burrs on the trimmed sample with the local chippings sites on the lower trimming tool

? Hole Expansion
Test (ISO 16630)

? Tensile Test of
Samples with One
Sheared Edge

? Side-Bending Test


No Visible Sources of Fracture
Cracks Forming in the Central Area
Cracks are Visible in Multiple Locations
Throughout the Thickness

No Visible Sources of Fracture
Cracks Forming in the Central Area
Cracks are Visible Throughout the Thickness
Including Burr Side and Burnish Side

No Visible Sources of Fracture

Hairline Cracks Seen in Burr Zone
Macro Cracks Propagating from the Burr Zone

The Burr affected zone (broken burr and burr formation) is 30%mof the gauge length.


If the localized necking coincides with the burr affected zone, the sample fails similarly to the high clearance samples (>20%), which have the entire length affected by the burr.


? DP980 shows lower tendency to form burrs in trimming due to breaking them off at the end of the trimming process;

? Chipping of the lower die prevails as a die wear mechanism for D2 inserts in trimming of DP980; and

? Avoiding burr formation helps to maintain sheared edge stretchability of DP980 throughout the life of the tool.

? Among reviewed methods to measure sheared edge stretchability, in-plane side bending of the strip with the sheared edge seems to have high potential for industrial applications.


1. Chintamani, J. and Sriram, S., "Sheared Edge Characterization of Steel Products used for Closure Panel Applications," SAE Technical Paper 2006-01-1589, 2006, doi:10.4271/2006-01-1589.

2. Konieczny, A. and Henderson, T., "On Formability Limitations in Stamping Involving Sheared Edge Stretching," SAE Technical Paper 2007-01-0340, 2007, doi:10.4271/2007-01-0340.

3. Coryell, J.J. “Edge Fracture in Mixed Microstructure Steels,” GDIS 2016

4. Zhou, D., Du, C., Hsiung, G., and Schmid, K. “Lessons Learned from Ultra High-Strength Steel Blanking,” GDIS 2015.

5. Golovashchenko, S.F. and Ilinich A.M., Analysis of trimming processes for stamped body panels, GDIS 2008.

6. Le, Q.B., deVries, J.A., Golovashchenko, S.F., and Bonnen, J.J.F., “Analysis of sheared edge formability of aluminum,“ Journal of Materials Processing Technology 214 (2014) 876– 891.

7. Nasheralahkami, S., Golovashchenko, S.F., Malek,C., Rugh, E., Kowalsky, D. and Zhou, W., “Sheared Edge Stretchability of Steels Suitable for Automotive Applications,” SAE Paper 2017-01-1708.

8. Nasheralahkami, S., Golovashchenko, S.F., Dawson, S.A., Sohmshetty, R. “Analysis of Tool Wear for Trimming of DP980 Sheet Metal Blanks,” 2017 SAE International doi:10.4271/2017-01-0302.

9. Nasheralahkami, S., Golovashchenko, S., Pan, K., Brown, L. et al., "Characterization of Trimmed Edge of Advanced High Strength Steel," SAE Paper .




Write a Comment
Three plus Five =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 亚洲午夜国产精品无码老牛影视| 亚洲色精品vr一区二区三区| 在线无码va中文字幕无码| 成人无码av一区二区| 国产蜜臀av在线一区尤物| 天天躁夜夜躁狠狠久久| 色偷偷噜噜噜亚洲男人| 国产精品无码无片在线观看 | 农村乱人伦一区二区| 男人和女人高潮做爰视频| 亚洲欧美日韩成人综合网| 亚洲欧美闷骚影院| 99久久国语露脸精品国产色| 国产对白国语对白| 午夜性爽视频男人的天堂| 亚洲偷偷自拍高清| 丰满大乳少妇在线观看网站| 亚洲精品久久久打桩机| 精品久久久久久久国产潘金莲| 乱人伦无码中文视频在线| 无码高潮少妇毛多水多水免费| 亚洲欧洲日产国码久在线| 18禁黄网站禁片免费观看| 国产永久免费高清在线观看 | 国产精品国产三级国av在线观看 | 国产亚洲精品久久久久久武则天| 亚洲精品国产情侣av在线| 国产两女互慰高潮视频在线观看| 性高湖久久久久久久久| 亚洲色成人网站在线观看| 亚洲日本va午夜在线电影| 国产av明星换脸精品网站| 亚洲人人玩人人添人人| 亚洲国产欧美不卡在线观看 | 免费国产在线精品一区二区三区| 精品夜夜澡人妻无码av蜜桃| 午夜精品乱人伦小说区| 亚洲精品成人网站在线| .精品久久久麻豆国产精品| 岛国在线无码高清视频| 国产愉拍91九色国产愉拍|