高跟肉丝少妇A片在线-青青青国产在线观看免费-亚洲欧美另类在线图片区-欧美又粗又大xxxxbbbb疯狂-亚洲熟女少妇一区二区

Gas Metal Arc Welding of Advanced High- Strength Steels

2018-10-26 09:49:00
LUQIMENG
Original
2641

? Min Kuo, ArcelorMittal
? Tom Natale, AK Steel Corporation
? Stephen Tate, AK Steel Corporation
? Hassan Ghassemi, ArcelorMittal
? Elliot Biro, ArcelorMittal
? Amanda Scherzer, FiatChryslerAmerica US LLC
? Doug Howe, Ford Motor Company
? Mike Palko, Ford Motor Company
? Richard Carlson, General Motors
? Weiping Sun, Nucor Corporation
? Chonghua (Cindy) Jiang, AET Integration Inc.
? Justin Hunt, AET Integration Inc.
? Donald F. Maatz, Jr. R&E Engineering Services
? Daniel L. Galiher, Tower International
? Vaidyanath B. Rajan, Lincoln Electric
? Richard Paul, Auto/Steel Partnership
? The objective of this project is to evaluate the effects of gas metal arc welding (GMAW) and gas metal arc brazing (GMAB) on AHSS and UHSS and to identify the impact of welding on joint strength and microhardness.
? Tests include X-ray inspection, micro hardness, quasi-static shear tension, and metallurgical cross-sections. Selected thin gauge steels were joined using both GMAW and GMAB. referencing ISO 17636-2 and ISO 5817.
? Cross-sections were taken from the welded and brazed plates. The microhardness indent spacing was 0.2 mm.
? Quasi-static shear tension testing was conducted to obtain nominal stress-displacement curves. Nominal stress was calculated as the load divided by the coupon cross-sectional area. Actual weld or braze geometry was not considered in the nominal stress value. Tests were conducted at 5.0 mm/min.
? X-ray inspections were conducted on all zinc coated materials,


? Steel grades obtained from the A/SP Sample Bank include the following:
? 0.67 mm BH210 HDGI
? 0.65 mm BH240 HDGI
? 0.69 mm DP490 HDGA
? 2.00 mm DP780 HDGI
? 2.53 mm CP780 HDGI
? 2.70 mm 780SF Uncoated
? 1.95 mm DP980 HDGA
? 1.38 mm DP1180 Uncoated
? 1.40 mm DP1180 EG
? 1.40 mm MS1700 Uncoated



Steel sheets were
sheared to 6” x 12”
and welded in a lap
joint configuration
along the 12”
length. Test
specimens were
waterjet cut from
the center of the
welded plates, in
order to avoid the
weld start and stop
locations.
Specimen length
was parallel to the
sheet rolling
direction.


Welded and brazed joints were
produced using an OTC DP400
power supply with an OTC Almega
AX-V6 robot. Both DC constant
voltage (GMAW) and DC pulsed
(GMAW-P) processes were used,
depending on the material
thickness and coating. All welds
were made in the 1F position.

? Lincoln SuperArc L56 (ER70S-6), Lincoln SuperArc LA-90 (ER80S-D2), and
? Lincoln SuperArc AK-10 (ER100S-G) steel filler were used with 90% argon 10%CO2 shielding gas for GMAW joints.
? Luvata LuvaWeld S1 (CuSi-A) silicon bronze filler was used with 100% argon shielding gas for GMAB joints.



Zinc coated steels were welded with lower travel speed than uncoated steels in order to reduce porosity. For thin zinc coated steels, it was found that the L2 leg length needed to be greater than the targeted 2.5t. Low current and the fastest feasible travel speeds were attempted in order to minimize heat input for all materials.




High quality joints were achieved with all materials. 

With appropriate parameters and sheet gaps targeted at 0.1 mm, zinc coated materials were able to be joined with minimal porosity. 

Coated materials exhibited moderate degrees of spatter. This is likely caused by the low current and voltage levels required to produce small weld sizes.



Minor porosity was observed in the weld or braze metal of zinc coated materials. The highest area percent porosity was 1.98%, as determined from X-ray images.


? Quality welded and brazed joints were achieved with all test materials
? The current practice consisting of mechanical, metallographic, X-ray, and microhardness testing quantifies joint characteristics and could be used as a GMAW and GMAB qualification procedure
? Zinc coated steels were able to be welded with average area percent porosity less than 2% using appropriate welding schedules and the test conditions used in this study
? Sheet gaps targeted at 0.1 mm were shown to minimize porosity
? Fractures occurred in the base metal, HAZ, weld metal, or near the weld fusion line,depending on material grade and thickness
? Joint efficiency ranged from 41% (MS1700 Uncoated GMAW) to 105% (BH240 HDGIGMAB)
? Nominal joint strength ranged from 357 MPa (BH210 HDGI GMAW) to 788 MPa (DP1180 uncoated GMAW).


? Of the 780 MPa tensile strength materials tested, ER100S-G filler increased nominal joint strength for both CP780 HDGI and DP780 HDGI compared to ER70S-6 filler
? Fracture location did not necessarily correspond to the areas with the lowest microhardness
? Fracture location may be dependent on the stress concentration at the weld root, microhardness distribution and microstructure difference (metallurgical notch)
? For BH210 HDGI and BH240 HDGI, fracture occurred in the heat-affected zone close to the weld for steel filler and in the base metal away from the joint for silicon bronze filler
? DP490 HDGA joints welded with steel filler fractured outside of the weld metal and provided close to 100% joint efficiency
? For DP490 HDGA brazed with silicon bronze filler, fractures occurred in the softer braze metal, with average joint efficiency approximately 91%
? Joint efficiency generally decreased as steel strength increased




Write a Comment
Ten minus Nine =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 亚洲人成电影在线播放| 日本精品一区二区三区四区| 色香阁综合无码国产在线| 国内精品国内精品自线一二三区| 久久精品国产99国产精2021| 国产乱xxxxx97国语对白| 最新的国产成人精品2021| 性欧美熟妇videofreesex| 婷婷六月在线精品免费视频观看| 亚洲情a成黄在线观看| 大地资源在线播放观看mv| 精品国产一区二区三区2021| 乱色欧美激惰| 亚洲色大成网站www在线| 色综合av社区男人的天堂| 性夜久久一区国产9人妻| 午夜羞羞影院男女爽爽爽| 精品无码国产av一区二区三区 | 久久精品国产一区二区无码| 中文在线8资源库| 亚洲精品你懂的在线观看| 2021无码最新国产在线观看| 亚洲精品乱码久久久久久v| 婷婷激情综合色五月久久竹菊影视| 亚洲欧美18岁网站| 久久天天躁夜夜躁狠狠| 人妻无码| 国产精品中文久久久久久久| 无码不卡av东京热毛片| 亚洲成a人片在线不卡一二三区| 欧洲成人午夜精品无码区久久| 99久久精品无码一区二区三区 | 亚洲色成人网站www永久男男| 中文字幕日本最新乱码视频| 日韩欧美国产aⅴ另类| 韩国午夜理伦三级在线观看仙踪林 | 午夜亚洲影院在线观看| 99国产精品国产精品九九| 欧美日韩精品一区二区三区不卡| 欧美黑人与白人精品a片 | 在线观看无码av网址|